electroless prenickel - pH adjustment without ammonia 

                                                        

 

temperature 40°C + / - 5

pH 8.5 to 10,0

4,5 g/l nickel 15.0 g/l sodium hypophosphite

after 10 to 20 minutes of coverage of with zincate treated aluminum

prevents zinc pollution in electroless nickel bath

thus bath stability of electroless nickel baths improves

longer life span of electroless nickel baths

minimization of problems in quality - for example blisters

good adhesion of following layers

pH correction with 500 g/l KOH or 500g/l K2CO3

 

 

 

 

 

 